复合材料科学与工程 ›› 2013, Vol. 0 ›› Issue (7): 24-27.

• 基础研究 • 上一篇    下一篇

不同龄期下SHCC拉伸性能试验测定与分析

胡春红1, 高艳娥1, 王小成2   

  1. 1.河南理工大学土木工程学院,河南焦作 454003;
    2.河南鹏程路桥建设有限公司,河南焦作 454003
  • 收稿日期:2012-11-20 出版日期:2013-10-28 发布日期:2022-03-15
  • 作者简介:胡春红(1976-),女,博士,副教授,主要从事结构加固与修复。
  • 基金资助:
    河南理工大学青年基金(Q2010-13); 河南理工大学创新基金(Q2011-46)

EXPERIMENTAL MEASUREMENT AND ANALYSIS OF TENSILE PERFORMANCE OF SHCC IN DIFFERENT AGES

HU Chun-hong1, GAO Yan-e1, WANG Xiao-cheng2   

  1. 1. School of Civil Engineering,Henan Polytechnic University, Jiaozuo 454003,China;
    2. Henan Pengcheng Road&Bridge Co.,Ltd.,Jiaozuo 454003,China
  • Received:2012-11-20 Online:2013-10-28 Published:2022-03-15

摘要: 直接拉伸试验是最能反映SHCC 材料应变硬化与多微开裂特性的可行性试验,也是获得材料单轴拉伸应力-应变曲线的唯一可行方法。本文拟通过对不同龄期下每组三个试件进行直接拉伸试验,获得SHCC应力-应变全曲线,并在试验过程中观察不同龄期试件的裂缝发展情况。研究结果表明:任何龄期下的试件均表现出明显的应变硬化特性,且其极限拉应变均能达到甚至超过3%;不同龄期下试件的裂缝间距不同,即开裂特性有所差别; 随着龄期的增加,试件强度提高而韧性有所下降。本文所得结果可为该材料在实际工程中的推广应用提供理论指导。

关键词: SHCC, 应变硬化, 应力-应变曲线, 多微开裂, 龄期

Abstract: Direct tensile test is feasible to reflect the strain-hardening and multiple micro cracking characteristics of SHCC, it is also the only feasible method to get stress-strain curve of material on uniaxial tensile load. The stress-strain full curves of SHCC at different ages was obtained on the basis of direct tensile test in this paper, and crack development of different specimens was observed in the course of the experiments with three specimens each group. The results show that obvious strain hardening characteristics appears in all specimens, and the ultimate tensile strain can all reach or even exceed 3%, the crack spacing of specimens are various at different ages, the cracking characteristics have differences. With the increase of age, the tensile strength increases and the toughness decreases. The results obtained in this paper can provide theoretical guidance for the popularization and application of SHCC in the practical engineering.

Key words: SHCC, strain hardening, stress-strain curve, multiple micro cracking, age

中图分类号: